Two production routes

Cold-formed angle is made by roll forming or press braking strip into an L section. The corners are sharp, the leg dimensions hold a tighter tolerance, and the surface inherits the finish of the strip — so 2B or BA strip gives a clean, bright angle.

Hot-rolled angle is rolled in a mill with rounded corners and a wider dimensional tolerance, supplied pickled or as-rolled. It is heavier per metre for the same leg size and cheaper per tonne, which is why it dominates structural work where appearance is secondary.

For visible architectural work — handrail supports, balustrade frames, cladding sub-structures — cold-formed is usually the right call. For structural frames carrying load, hot-rolled is normal and the drawing will usually say so.

Dimensions and tolerance

Angle is specified by leg length × leg length × leg thickness, and by whether the legs are equal. Squareness of the corner, straightness and the tolerance on leg length all affect fabrication: an angle that is not square twists when welded into a frame, and the error is difficult to pull out afterwards.

European dimensioning follows EN 10056; where the drawing references a Chinese or Japanese standard, quote to that standard rather than converting.

Welding stainless angle

Austenitic stainless is readily welded by TIG, MIG or stick, but three things differ from carbon steel. Thermal expansion is higher, so shrinkage forces are larger. Thermal conductivity is lower, so heat concentrates at the joint. And the weld zone loses corrosion resistance unless heat tint is removed.

Use 304L or 316L rather than the standard-carbon grades where the frame will be welded and cannot be annealed afterwards. Clean the joint before welding — cutting oil and marking ink cause porosity — and remove heat tint by pickling or, at minimum, by pickling paste on the weld and heat-affected zone.

Controlling distortion

Distortion control is a sequence problem, not a material problem. Weld in a balanced order, alternating sides of the frame; clamp or jig the assembly until it has cooled; avoid weaving passes that put more heat into the section; and where the frame must be flat, weld the least critical joints first and check squareness between passes.

For thin legs, backing gas on the reverse side prevents oxidation and improves the root. For visible work, plan the polishing step after welding rather than before.

What to put on the order

  • Grade and standard, for example "316L to EN 10088-3".
  • Leg length × leg length × thickness, equal or unequal legs.
  • Length, and whether cut to length is required.
  • Process: hot rolled or cold formed, and the finish (pickled, 2B, polished).
  • Straightness and squareness tolerance for frame work.
  • Mill certificate to EN 10204 3.1.