The four supply conditions

Hot rolled bar comes straight from the mill with scale and a relatively loose diameter tolerance; it is the cheapest form and is used where the part is machined all over. Annealed bar has been heat treated to soften it and relieve stress, which improves machinability and dimensional stability.

Cold drawn bar is pulled through a die, producing a tight diameter tolerance, a smooth surface and higher strength from cold work. Ground bar is cold drawn and then centreless ground to the tightest tolerance and best finish — the standard stock for automatic screw machines and for shafting that runs in a bearing.

A fifth option, peeled or turned bar, machines away the surface layer to remove defects while keeping a softer condition; it is common for forging stock and for large diameters where grinding would be uneconomic.

Tolerance classes

Diameter tolerance is the number that decides whether the bar can be fed into a bar feeder without adjustment. Two bars of identical nominal diameter can differ by tenths of a millimetre between tolerance classes, and that difference is the whole reason a shop pays more for ground stock.

Straightness and length tolerance belong on the order as well: bent bar jams bar feeders, and short lengths cost more per kilogram because of the handling.

Machinability and the 303 trade-off

Austenitic stainless work-hardens, which is why it machines poorly compared with carbon steel. Free-machining grades such as 303 add sulphur to break the chip, raising cutting speed substantially. The cost is real: 303 is not recommended for welding, and its corrosion resistance is below 304 because the sulphide inclusions act as initiation sites for pitting.

Use 303 for high-volume turned parts that will not be welded and are not exposed to chlorides. For anything welded, or anything in a marine or chemical environment, stay with 304 or 316L and accept the slower cutting.

Standards and designation

ASTM A276 covers hot-finished and cold-finished stainless bar for general use. ASTM A479 covers bar and forging stock for boilers and pressure vessels, with additional testing. ASTM A582 covers free-machining grades. In European practice EN 10088-3 governs.

As with pipe, the standard decides the test regime, so a certificate that says "304" without naming the standard is not a complete answer for pressure or safety-critical work.

Bar for forging

Forging stock needs internal soundness more than surface finish. Specify peeled or turned bar where surface defects would be carried into the forging, and state the forging ratio and any ultrasonic inspection requirement. For high-temperature alloys, the condition and grain size may also be specified.

What to put on the order

  • Grade, standard and condition: for example "316L to ASTM A276, cold drawn and ground".
  • Diameter with tolerance class; shape (round, square, hex, flat).
  • Length and straightness tolerance.
  • Surface requirement: black, pickled, turned, ground, polished.
  • Hardness or heat-treatment condition where the part is machined to a final property.
  • Mill certificate to EN 10204 3.1, with heat number marked on the bundle.